| Material | Recommended Product | Service Temperature (° C) | |||
|---|---|---|---|---|---|
| 70 | 90 | 105 | 125 | ||
| PVC ( k=65 to 71 ) | – | 100 | 100 | 100 | 100 |
| Plasticizer | DOP/DINP | 45 – 60 | – | – | – |
| Plasticizer | DIDP | – | 15 | – | – |
| Plasticizer | TOTM | – | 2 – 35 | 30 – 50 | 35 – 50 |
| Epoxy Soybean Oil | Alpex 5-6 | 0 – 5 | 0 – 5 | 0 – 5 | 0 – 5 |
| Filler | Calcium Carbonate | 40 – 60 | 5 – 25 | – | – |
| Filler | Kaolin | – | – | 10 – 15 | 5 – 10 |
| Retardant | Antimony Trioxide | – | 0 – 5 | 3 – 6 | 3 – 6 |
| External Lubricant | Pe-Wax | 0 – 0,6 | 0 – 0,2 | 0 – 0,2 | 0 – 0,2 |
| Ca/Zn Based Stabilizer | Akropan 25xx/26xx – Class 1 | 3,5 – 5 | 5,5 – 7,5 | 7 – 10,0 | 13,5 – 15 |
| Material | Recommended Product | Sheating | Service Temperature (° C) | |||
|---|---|---|---|---|---|---|
| 70 | 90 | 105 | 125 | |||
| PVC ( k=65 to 71 ) | – | 100 | 100 | 100 | 100 | 100 |
| Plasticizer | DOP/DINP | 45 – 60 | 40 – 60 | – | – | – |
| Plasticizer | DIDP | – | – | 15 | – | – |
| Plasticizer | TOTM | – | – | 20 – 35 | 35 – 50 | 35 – 50 |
| Epoxy Soybean Oil | Alpex 5-6 | 0 – 5 | 0 – 5 | 0 – 5 | 0 – 5 | 0 – 5 |
| Filler | Calcium Carbonate | 60 – 100 | – | 5 – 25 | – | – |
| Filler | Kaolin | – | 30 – 50 | – | 10 – 15 | 5 – 10 |
| Retardant | Antimony Trioxide | – | – | 0 – 5 | 3 – 6 | 3 – 6 |
| External Lubricant | Pe-Wax | 0 – 0,6 | 0 – 0,6 | 0 – 0,2 | 0 – 0,2 | 0 – 0,2 |
| Pb Based Stabilizer | Akropan 21xx | 3,5 – 5 | 3 – 3,8 | 5 – 7 | 7 – 10 | 9 – 12 |